alloygen.charge_calc/1Data under reviewCharge
Input: 40X, 800 kg, your stock
Charge for 40X in furnace IF_1T: 799.8 kg tapped, 41.6 UAH per kg of good casting.
- Tapped
- 799.8 kg
- Charged
- 824.5 kg
- Per kg of good casting
- 41.6 UAH
- Heat total
- 21,625 UAH
Charge in addition order
| # | When | Material | Mass | Cost |
|---|---|---|---|---|
| 1 | on the hearth, before charging | GRAPH carburizer | 3.0 kg | 78 UAH |
| 2 | charging | SCRAP_CLEAN scrap | 807.0 kg | 11,702 UAH |
| 3 | after the charge has melted | FECR ferroalloy | 10.5 kg | 1,239 UAH |
| 4 | after the charge has melted | FEMN ferroalloy | 2.5 kg | 205 UAH |
| 5 | after the charge has melted | FESI ferroalloy | 1.5 kg | 108 UAH |
| Charge total | 824.5 kg | 13,332 UAH |
Expected analysis vs the grade field, wt %
| Element | Grade field | Expected | Status |
|---|---|---|---|
| C | 0.36–0.44 | in field | |
| Si | 0.17–0.37 | in field | |
| Mn | 0.5–0.8 | in field | |
| Cr | 0.8–1.1 | in field | |
| Ni | ≤ 0.3 | in field | |
| Cu | ≤ 0.3 | in field | |
| P | ≤ 0.035 | in field | |
| S | ≤ 0.035 | in field |
Assumptions, warnings and sources
Warnings
- Mediumgrade 40X limits are checked against secondary sources, not the text of GOST 4543-2016 / DSTU 7806:2015 (table 1 as quoted elsewhere; the standard itself was not read). Not enough for a certificate.
- Mediumbrittle temperature range LIT–ZDT 45 °C (at 1 °C/s); sulphur and phosphorus account for 28 °C (63%) of it: they segregate into the liquid between dendrites (at fs = 0.9: S 0.128%, P 0.116%). With S 0.00785% and P 0.00975% the range narrows to 31 °C. In a furnace without refining this is done only through the charge: scrap and ferroalloys lower in sulphur and phosphorus.
- Mediumno product requirements given: there is nothing to select a grade by, so the calculation runs only for the grade named explicitly.
- Mediumprices of 4 charge items have no price list or date (FECR, GRAPH, FEMN, FESI): the cost estimate is a demo — add your dated price list.
- Mediumelement recovery in furnace IF_1T is a reference value, not derived from heat history. The expected analysis will differ from the ladle sample more, the more silicon, manganese, aluminium and titanium the charge has.
- Mediumthe tariff of 8.5 UAH/kWh is not backed by a bill or contract — set your own tariff.
- NoteCE(IIW) = 0.65 > 0.45: welding will need preheating.
Assumptions
- The charge aims at the working window — the central 70% of each element's tolerance field, leaving room for analysis scatter.
- Grade 40X limits come from the alloygen grade book via secondary sources (GOST 4543-2016, table 1); not checked against the official text — pilot, under review.
- Charge compositions, prices and stock are the foundry's data; the service computes with them and does not verify them (warnings say where an item has no document).
- Melting loss uses element recovery for furnace IF_1T (induction): reference values, not calibrated on this furnace's heat history.
- Cost: charge at stock prices plus energy, lining and conversion from furnace data; lines and totals are in the response.
Sources
- GOST 4543-2016 / DSTU 7806:2015 — structural alloy steel products, grades (via secondary sources)as of Oct 5, 2026 Data under review
- SCRAP_CLEAN price: foundry invoice No. 118as of Sep 20, 2026